VKA ACHIEVES 1.43% V2O5 & 59% FE IN HIGH QUALITY CONCENTRATE
Released
Released
Announcement PDF
ASX ANNOUNCEMENT
6 March 2024
VKA ACHIEVES 1.43% V2O5 & 59% FE IN HIGH QUALITY
CONCENTRATE
•
Viking Mines has received excellent results for Low Intensity Magnetic Separation
(“LIMS”) testwork conducted on bulk concentrate produced as part of the Stage 2
Metallurgical Testwork.
•
LIMS separation uses laboratory scale techniques using the same technical methods
which would be employed at an operating mine and is used as an indication of what
can be achieved.
•
The LIMS process delivered a high-quality concentrate grading 1.43% V2O5, 59% Fe
& 11.7% TiO2.
•
Maintaining Fe above 58% is a key achievement, as it demonstrates that the
significant value of contained iron in the Canegrass Project has the potential to be
realised as a saleable magnetite concentrate.
•
Total recovery of V2O5 is excellent at 93.0% from ore feed and Fe is high at 83.7%.
•
A high mass recovery of 53.2% was achieved, meaning for every 1kg of sample,
0.532kg of concentrate is produced. This has real world impacts for limiting the size
(and capital cost) of the milling operation required to produce the concentrate.
•
Silica and Alumina combined are 3.8%, which is comfortably below the threshold
target of 4% for roasting (which is the next step required to produce V2O5 flake).
•
Nickel, Copper & Cobalt report to the tail (non-magnetic fraction) with grades of
0.089%, 0.115% and 0.027% respectively. Further testwork is planned to determine
if a sulphide concentrate of these commodities can be produced from this material.
•
Sighter roasting testwork has commenced which will determine the key parameters
(temperature and duration) and reagents to be used ahead of producing V2O5 flake.
Viking Mines Limited (ASX: VKA) (“Viking” or “the Company”) is pleased to provide an
update on the ongoing metallurgical progress at the Company’s flagship Canegrass Battery
Minerals Project (“the Project” or “Canegrass”), located in the Murchison Region of Western
Australia.
Further results have been received for the ongoing Stage 2 metallurgical testwork on samples
collected from the Fold Nose deposit within the Canegrass Project.1
A high-quality magnetite concentrate has been produced via LIMS methodology grading
1.43% V2O5, 59% Fe and 11.7% TiO2. Recoveries from the ore are high at 93.0%, 83.7% and
79.5% respectively, with an overall mass pull of 53.2%.
Importantly, SiO2 and Al2O3 has a combined total of 3.8%, which is below the threshold of 4%
required for roasting of the concentrate to liberate the V2O5.
Sighter roasting testwork on the concentrate has commenced to determine the final roasting
parameters to be used to produce V2O5 flake.
1
Viking Mines (ASX:VKA) ASX Announcement 15 December 2023 – Stage 2 Met Testwork Update
ASX:VKA
vikingmines.com
15-17 Old Aberdeen Place
West Perth, WA, 6005
P +61 8 6245 0870
F +61 8 9322 5230
contact@vikingmines.com
1
Commenting on the progress of the Stage 2 metallurgical testwork, Viking Mines
Managing Director & CEO Julian Woodcock said:
“I’m extremely pleased with the performance of the samples and the progress made with the
metallurgical testwork.
“The quality of the concentrate delivers on our expectations with high recoveries of the primary
commodities, high mass pull and low silica and alumina required to proceed with roasting.
“We have maintained the high vanadium recoveries seen in the sighter Davis Tube Recovery
(“DTR”) testwork with 93.0% and significantly reduced the silica and alumina content which is
critical for the project to proceed on a conventional processing pathway.
“The next key step will be to produce V2O5 flake from the concentrate and then we will have
demonstrated a pathway to unlocking the significant value of this substantial Resource.
“We will also continue to investigate options to further enhance the value of the Project such as
producing a sulphide concentrate from the tail to realise value of the significant Cu, Ni & Co
credits, separating the Fe and Ti to produce a premium magnetite concentrate and ilmenite
(titanium) concentrate and finally targeting a high purity >99% V2O5 flake product which attracts
a premium for use in the electrolyte, aerospace, and defence industries.
“Viking are rapidly advancing this high-value Project, and when this testwork is complete we will
be able to assess the true value which can be realised for the benefit of our shareholders. I look
forward to sharing the progress and results with the market as we achieve key milestones.”
Stage 2 Metallurgical Testwork Programme
Testwork commenced in December 2023 on samples collected from the Fold Nose deposit at
the Project. Samples are composited ahead of producing a magnetic concentrate before
further processing to produce high purity V2O5 flake along with other marketable products
including >58% Fe Magnetite Concentrate and Cu, Ni, Co sulphide concentrates.
To date, the wet magnetic separation steps have been optimised and completed to produce
a high-quality magnetic concentrate suitable for proceeding with roasting testwork.
The laboratory has provided an update on the timing for completion of the testwork. There
have been delays of approximately 4 weeks, and the revised completion date for all steps is
now forecasted for April 2024. The Company will continue to provide updates on progress
throughout this period as results are received.
Wet Magnetic Separation
A multi-step process using Low Intensity Magnetic Separation (“LIMS”) was followed to
produce a high-quality magnetic concentrate suitable for advancing to the next step of
roasting testwork.
Initially a bulk concentrate was produced using Bulk Rougher LIMS process at a grind size of
P80 145 micron. A very high mass recovery of 64.2% was achieved at this stage of the process.
The concentrate graded 1.18% V2O5, 50% Fe, 10.7% TiO2 and yielded a combined Silica and
Alumina of 11.3%.
18kg of the rougher concentrate was subsequently ground to P80 45 micron and processed
using a 3 stage Bulk Cleaner LIMS process to achieve target concentrate quality suitable for
roasting. 14.9kg of magnetic concentrate was produced through this process, representing a
final mass recovery of 53.2% from the original sample. Results and quality of concentrate for
each of the stages are provided in Table 1 and Table 2, and photos of the LIMS process in
Figure 1.
ASX:VKA | vikingmines.com
2
The concentrate has the following key characteristics:
•
A high-quality magnetic concentrate has been produced from Canegrass ore using LIMS
methodology and meeting key quality parameters.
•
High mass recovery achieved of 52.8%.
•
Concentrate grades are high with V2O5 1.43%, Fe 59% & TiO2 11.7%.
•
Metal recoveries to concentrate are high with 93.0%V2O5, 83.7% Fe and 79.5% TiO2.
•
Combined silica and alumina levels are low at 3.8% and critically, meeting the requirement
for roasting of <4%.
•
Ni, Cu and Co report to the tail in the concentrate process, with recoveries of 69.7%, 72.8%
and 64.3% respectively. This presents the opportunity for further testwork to recover these
valuable commodities by performing a standard sulphide floatation process on the tail
which will be investigated further.
Table 1; Magnetic concentrate results showing mass recoveries and grades at each step of the LIMS process. Cleaner 3 mags is the
final concentrate produced.
Table 2; Metal recoveries for each of the magnetic concentrates and tail for each of the LIMS stages.
ASX:VKA | vikingmines.com
3
Figure 1; Photos showing A) Samples being prepared for filtration after DTR testwork completed, B) Eirez Davis Tube
tester setup for sighter DTR testing and C) Magnetic concentrate produced after filtration.
NEXT STEPS
Based on the results received, the Company’s metallurgical consultants have determined the
next stage of the testwork as follows. This work has commenced, and the Company will
continue to provide updates as further results are received.
•
Complete 16 sighter roasting tests using various combinations of roasting time,
temperature and reagents to determine optimum roasting conditions for Canegrass Ore.
•
Leach sighter roasting products using water to dissolve liberated vanadium into solution
and assay.
•
Once optimum roasting conditions determined, undertake bulk roasting testwork on a
larger sample to produce sufficient product for purification testwork.
•
Complete purification process to produce minimum of 98% V2O5 flake product.
•
Investigate options for further refining purification process to produce high purity >99%
V2O5 flake product.
•
Investigate options to improve concentrate Fe grade to 62%.
•
Investigate options to separate the TiO2 into a separate concentrate for options a separate
product.
ASX:VKA | vikingmines.com
4
•
Develop test plans for floatation testwork on tail residues from magnetic concentrate
process to determine if Ni, Cu and Co can be recovered into sulphide concentrates.
END
This announcement has been authorised for release by the Board of the Company.
Julian Woodcock
Managing Director and CEO
Viking Mines Limited
For further information, please contact:
Viking Mines Limited
Michaela Stanton-Cook - Company Secretary
+61 8 6245 0870
Forward-Looking Statements
This document may include forward-looking statements. Forward-looking statements include, but are not limited to, statements concerning Viking
Mines Limited’s planned exploration programme and other statements that are not historical facts. When used in this document, the words such as
"could," "plan," "estimate," "expect," "intend," "may”, "potential," "should," and similar expressions are forward-looking statements. Although Viking
Mines Limited believes that its expectations reflected in these forward-looking statements are reasonable, such statements involve risks and
uncertainties and no assurance can be given that actual results will be consistent with these forward-looking statements.
Competent Persons Statement – Metallurgical Results
The information contained in this report, relating to metallurgical results, is based on, and fairly and accurately represent the information and
supporting documentation prepared by Mr Damian Connelly. Mr Connelly is a full-time employee of METS Engineering who are a Contractor to
Viking Mines Ltd, and a Fellow of The Australasian Institute of Mining and Metallurgy. Mr Connelly has sufficient experience which is relevant to the
style of mineralisation and type of deposit under consideration, and to the activity being undertaken to qualify as a Competent Person as defined in
the 2012 Edition of the Australasian Code for Reporting of Exploration Results, Exploration Targets, Mineral Resources and Ore Reserves. Mr Connelly
consents to the inclusion in the report of the matters based on the results in the form and context in which they appear.
Competent Persons Statement – Exploration Results
Information in this release that relates to Exploration Results is based on information compiled by Mr Julian Woodcock, who is a Member and of the
Australian Institute of Mining and Metallurgy (MAusIMM(CP) – 305446). Mr Woodcock is a full-time employee of Viking Mines Ltd. Mr Woodcock has
sufficient experience which is relevant to the style of mineralisation and type of deposit under consideration and to the activity being undertaken to
qualify as a Competent Person as defined in the 2012 Edition of the ‘Australasian Code for Reporting of Exploration Results, Mineral Resources and
Ore Reserves’. Mr Woodcock consents to the disclosure of the information in this report in the form and context in which it appears.
Competent Persons Statement – Mineral Resources
The information in this announcement that relates to the Mineral Resource estimate is derived from information compiled by Mr Dean O’Keefe, a
Fellow of the Australasian Institute of Mining and Metallurgy (AusIMM, #112948), and Competent Person for this style of mineralisation. Mr O’Keefe
is a consultant to Viking Mines Limited, and is employed by MEC Mining, an independent mining and exploration consultancy. Mr O’Keefe has
sufficient experience relevant to the style of mineralisation and type of deposit under consideration and to the activity which he is undertaking to
qualify as Competent Person as defined in the 2012 edition of the Australasian Code for the Reporting of Exploration Results, Mineral Resources, and
Ore Reserves (JORC Code). The Company confirms that the form and context in which the results are presented and all material assumptions and
technical parameters underpinning the estimates in the original market announcement continue to apply and have not materially changed from the
original announcement and that the form and context in which the Competent Person’s findings are presented have not been materially modified
from the original announcement on 20 November 2023.
ASX:VKA | vikingmines.com
5
CANEGRASS BATTERY MINERALS PROJECT
The Canegrass Battery Minerals Project is located in the Murchison region, 620km north-east
of Perth, Western Australia. It is accessed via sealed roads from the nearby township of Mt
Magnet to within 22km of the existing Resources. The Project benefits from ~95km 2 of
exploration tenements, with a 7,500m resource drilling programme proving to be highly
successful upgrading the JORC (2012) Inferred Mineral Resource Estimate (MRE) to 146Mt at
0.70% V2O5, 31.8% Fe & 6.6% TiO2 (>0.5% V2O5 cut-off)6. Importantly, a high-grade subset of
the MRE has been calculated, totalling 27.5Mt at 0.87% V2O5, 37.3% Fe & 8.0% TiO2 (>0.8%
V2O5 cut-off)6, which the Company believes to be sufficient to commence a Scoping Study.
JORC (2012) MINERAL RESOURCE
The Canegrass Mineral Resource has been calculated across three separate areas called the
Fold Nose, Kinks and Kinks South deposits. The Resource has subsequently been reported
above a cut-off grade of 0.5% V2O5 and above the 210 RL (equivalent to a maximum depth of
~250m)(refer to ASX Announcement on 20 November 2023).
Canegrass Project Vanadium Mineral Resource estimate, 0.5% V 2O5 cut-off grade, >210m RL. (due to the effects of
rounding, the total may not represent the sum of all components).
Target Commodities
Deleterious Elements
JORC (2012) Cut-Off Tonnage
MRE
Ni
Co Al2O3 SiO2
P
V2O5 Fe TiO2 Cu
Classification V2O5%
(Mt)
%
%
%
%
%
%
%
%
%
VKA 2023 Model
Inferred
>0.5
146
0.70 31.8 6.6 0.066 0.062 0.016 11.7 21.7 0.005
LOI
%
1.7
VIKING MINES FARM-IN AGREEMENT
Viking, via its wholly owned subsidiary, Viking Critical Minerals Pty Ltd, commenced with a
Farm-In arrangement (FIA) with Red Hawk Mining Ltd (formerly Flinders Mines Ltd) (ASX:RHK)
on 28 November 2022 to acquire an equity interest in the Canegrass Battery Minerals Project.
Through the terms of the Farm-In, Viking can acquire up to 99% of the Project through
completion of 4 stages via a combination of exploration expenditure of $4M and staged
payments totalling $1.25M over a maximum period of 54 months. As of August 2023, Viking
has acquired 25% of the Project through the FIA.
If Viking complete the Farm-In to 99% equity interest, Red Hawk may offer to sell to Viking the
remaining 1% of the Project for future production and milestone related payments totalling
$850,000. If Red Hawk Mining do not offer to sell within a prescribed timeframe their right
lapses, they must offer Viking the right (but not the obligation) to buy the remaining 1% for the
same terms.
The Project has a legacy 2% Net Smelter Royalty over the project from when Red Hawk Mining
acquired it from Maximus Resources in 2009.
ASX:VKA | vikingmines.com
6
VANADIUM REDOX FLOW BATTERIES – GREEN ENERGY FUTURE
Viking Mines recognise the significant importance of Vanadium in decarbonisation through the
growth of the Vanadium Redox Flow Battery (“VRFB’s”) sector.
VRFB’s are a developing market as an alternate solution to lithium-ion (“Li-ion”) in specific large
energy storage applications. Guidehouse Insights Market Intelligence White Paperi published
in 2Q 2022 forecasts the VRFB sector to grow >900% by 2031 through the installation of large,
fixed storage facilities (Figure 24).
Figure 2; Forecast growth of the VRFB Sector through to 2031 (source – Guidehouse Insightsi)
The reason for this forecast growth is that VRFB’s have unique qualities and advantages over
Li-ion in the large energy storage sector to complement renewable energy sources to store the
energy produced. They are durable, maintain a long lifespan with near unlimited
charge/discharge cycles, have low operating costs, safe operation (no fire risk) and have a low
environmental impact in both manufacturing and recycling. The Vanadium electrolyte used in
these batteries is fully recyclable at the end of the battery’s life.
Importantly, and unlike Li-ion, the battery storage capacity is only limited by the size of the
electrolyte storage tanks. This means that with a VRFB installation, increasing energy storage
capacity is only a matter of adding in additional electrolyte (via the installation of additional
electrolyte storage tanks) without needing to expand the core system components. Increasing
the energy storage directly reduces the levelized cost per kWh over the installation’s lifetime.
This is not an option with Li-ion batteries.
It is for these reasons that VRFB’s are an ideal fit for many storage applications requiring longer
duration discharge and more than 20 years of operation with minimal maintenance.
i) Guidehouse Insights White Paper Vanadium redox Flow Batteries Identifying Market Opportunities and Enablers Published 2Q 2022
https://vanitec.org/images/uploads/Guidehouse_Insights-Vanadium_Redox_Flow_Batteries.pdf
ASX:VKA | vikingmines.com
7
APPENDIX 2 – JORC CODE, 2012 EDITION – TABLE 1
JORC Table 1, Section 1 – Sampling Techniques and Data
JORC Code explanation
Criteria
Sampling
techniques
Drilling
techniques
Nature and quality of sampling (e.g. cut channels, random chips, or specific specialised industry standard
measurement tools appropriate to the minerals under investigation, such as downhole gamma sondes, or
handheld XRF instruments, etc.). These examples should not be taken as limiting the broad meaning of
sampling.
Include reference to measures taken to ensure sample representivity and the appropriate calibration of any
measurement tools or systems used.
Aspects of the determination of mineralisation that are Material to the Public Report. In cases where ‘industry
standard’ work has been done this would be relatively simple (e.g. ‘reverse circulation drilling was used to obtain
1 m samples from which 3 kg was pulverised to produce a 30 g charge for fire assay’). In other cases more
explanation may be required, such as where there is coarse gold that has inherent sampling problems. Unusual
commodities or mineralisation types (e.g. submarine nodules) may warrant disclosure of detailed information
Drill type (e.g. core, reverse circulation, open-hole hammer, rotary air blast, auger, Bangka, sonic, etc.) and
details (e.g. core diameter, triple or standard tube, depth of diamond tails, face-sampling bit or other type,
whether core is oriented and if so, by what method, etc.).
Method of recording and assessing core and chip sample recoveries and results assessed.
Drill sample
recovery
Measures taken to maximise sample recovery and ensure representative nature of the samples.
Whether a relationship exists between sample recovery and grade and whether sample bias may have occurred
due to preferential loss/gain of fine/coarse material.
Whether core and chip samples have been geologically and geotechnically logged to a level of detail to support
appropriate Mineral Resource estimation, mining studies and metallurgical studies.
Logging
Whether logging is qualitative or quantitative in nature. Core (or costean, channel, etc.) photography.
ASX:VKA | vikingmines.com
Commentary
RC drilling collected samples during the drilling process using industry
standard techniques including face sampling drill bit and cone splitter.
Chip samples are collected from the drill cuttings and sieved and put
into chip trays for geological logging.
Cone splitter subsamples the interval drilled and ensures that the
sample collected is representative of the interval drilled.
Reverse circulation drilling was used to obtain 1m samples which were
collected from the cone splitter. Samples have been composited in
some cases to either 2 or 4m composites by scooping from the calico
bag collected from the cone splitter at the rig. Samples were
dispatched to ALS laboratories in Perth for analysis by a XRF fused bead
analysis.
Reverse circulation drilling using a 5 ½ inch bit and a face sampling
hammer.
Recovery of sample is recorded by the field assistant when sampling and
noted as either Good, Fair or Poor. Of the samples collected from the
drilling programme, very few samples reported fair or poor recovery and
no issues were identified with sample recovery for any samples related
to the mineralised horizons.
Drilling recovery is assessed by observing sample size. Samples are
collected from the cyclone using a cone splitter and monitored for size
to determine that they are representative.
No relationship has been identified between sample recovery and
grade. This is reflected by all samples collected having a good recovery.
Further, due to the nature of the mineralisation under investigation
and the relatively high values obtained, the impact of fines is not
considered to be of significance.
All chip samples have been geologically logged to a sufficient level to
support any future mineral resource estimation, mining studies and
metallurgical studies. All chip samples are retained at the Company
offices and are available for further inspection when undertaking this
future work.
Logging of samples is qualitative in nature. Chip photos are taken of the
chip trays. All the drill spoils at the drill site are photographed to retain
a record of the colour variation within the hole.
8
JORC Code explanation
Criteria
The total length and percentage of the relevant intersections logged.
If core, whether cut or sawn and whether quarter, half or all core taken.
If non-core, whether riffled, tube sampled, rotary split, etc. and whether sampled wet or dry.
For all sample types, the nature, quality and appropriateness of the sample preparation technique.
Subsampling
techniques and
sample
preparation
Quality control procedures adopted for all subsampling stages to maximise representivity of samples.
Measures taken to ensure that the sampling is representative of the in-situ material collected, including for
instance results for field duplicate/second-half sampling.
ASX:VKA | vikingmines.com
Commentary
All metres drilled have been geologically logged.
Not applicable.
Samples were collected from the cyclone using a cone splitter for each
metre drilled in to 2 calico bags. When composite samples were
collected, a scoop is used to collect equal amounts from each metre
interval used to make the composite sample. Dry samples are
collected.
For drill samples, The sample preparation of the RC samples follows
industry best practice, involving oven drying, pulverising, to produce a
homogenous sub sample for analysis. All samples were pulverised to a
nominal 85% passing 75-micron sizing and sub sampled for assaying
and LOI determination tests. The sample preparation techniques are of
industry standard and are appropriate for the sample types and
proposed assaying methods.
For metallurgical samples, calico bags from each of the 1m samples
under investigation were collected from the field and submitted to
Bureau Veritas. A master composite has been created using 1.5kg of
sample from each of the samples provided. 5x 150g splits of this
sample have undergone grind size and residence time testwork to
determine appropriate grind size for next stages of testwork. A further
portion of bulk master composite sample underwent a series of
magnetic separation steps to produce a clean magnetic concentrate.
Both head an tail samples at each of the stages were analysed to
determine their composition. Analysis results of the composite
compare closely to that of the mathematically composited interval
from the drilling analysis results, supporting the appropriateness of the
techniques used to produce the composite sample. The competent
person has determined that the sample preparation technique is
appropriate for the sample types.
For drill samples, standard, blank and duplicate samples are inserted in
the sampling sequence at a rate of 1 per 20 samples (standard or blank).
This is in addition to the laboratory QAQC procedures adopted. The
quality control procedures to ensure and maximise sample
representivity are deemed appropriate.
For metallurgical testwork, Laboratory standards were used in the
analysis of the composite sample and DTR testwork samples. No issues
have been reported by the laboratory.
Drilling was conducted using a 5 ½ inch hammer to collect 1m samples.
As the style of mineralisation is massive to disseminated with results
for V2O5 being measured in %, the samples collected are deemed
representative. To monitor this, duplicate samples are collected from
9
JORC Code explanation
Criteria
Whether sample sizes are appropriate to the grain size of the material being sampled.
The nature, quality and appropriateness of the assaying and laboratory procedures used and whether the
technique is considered partial or total.
Quality of assay
data and
laboratory tests
For geophysical tools, spectrometers, handheld XRF instruments, etc., the parameters used in determining the
analysis including instrument make and model, reading times, calibrations factors applied and their derivation,
etc.
Nature of quality control procedures adopted (e.g. standards, blanks, duplicates, external laboratory checks) and
whether acceptable levels of accuracy (i.e. lack of bias) and precision have been established.
ASX:VKA | vikingmines.com
Commentary
the cyclone at a frequency rate of approximately 1 per 40 samples
collected (~2.5%).Samples are selected from expected mineralised
intervals to provide meaningful data to compare the original vs the
duplicate. Duplicate samples show a good correlation against the
original sample collected indicating that sampling is representative of
the in-situ material collected.
No duplicate samples have been prepared as part of the metallurgical
testwork programme.
The Competent Person considers the current methods and processes
described as appropriate for this style of mineralisation.
Grind size establishment testwork for the metallurgical testwork
programme showed variable grind sizes but with no apparent influence
on recovery or grade.
The nature and style of the mineralisation is relatively homogenous
and as such the sample sizes collected are appropriate to the grain size
of the material being sampled.
For drill samples, Samples were sent to ALS laboratories in Perth for
preparation and analysis. Samples were riffle split to 250g then
pulverised to a nominal 85% passing 75 microns. The Vanadium
samples underwent analysis by ME-GRA5 (H20 LOI) and MEX-XRF21u
(iron ore by XRF fusion).
For metallurgical samples, samples were analysed by Bureau Veritas in
Perth. XRF-202 method and laser ablation techniques were used by
Bureau Veritas to analyse the samples.
The analysis methods chosen are considered appropriate for the style
of mineralisation and considered total.
Field tools were used to assist in identification of the VTM horizon for
sampling. A KT-10 magnetic susceptibility meter has been used which
measures the magnetic susceptibility of the sample. Unit specifications
are:
•
Circular coil design
•
Sensitivity: 10-6 SI units
•
Measurement range:
0.001 x 10-3 to 1999.99 x 10-3 SI units
No calibration factors are applied to the data. The duration for the
measurement sequence is 7 seconds.
As part of the drilling programme, a comprehensive QAQC programme
involving the insertion of standards (certified reference materials –
CRM’s), blanks and duplicates has been implemented. Viking inserts
standards at a frequency of 1:25, blanks 1:40 and duplicates 1:40. 3 x
CRM’s have been used by the Company which were sourced from
10
JORC Code explanation
Criteria
The verification of significant intersections by either independent or alternative company personnel.
The use of twinned holes.
Documentation of primary data, data entry procedures, data verification, data storage (physical and electronic)
protocols.
Verification of
sampling and
assaying
Discuss any adjustment to assay data.
Location of data
points
Accuracy and quality of surveys used to locate drillholes (collar and downhole surveys), trenches, mine workings
and other locations used in Mineral Resource estimation.
ASX:VKA | vikingmines.com
Commentary
GeoStats and are certified for 21 elements (including Vanadium) and
LOI. Results from the laboratory for the CRM’s are plotted against the
CRM values for the mean and 1,2, and 3 standard deviations from the
mean. 2 of the 3 standards all performed within expected levels with 1
standard demonstrating good precision and a minor positive bias for
accuracy. Further check assaying on 10 standards has been completed
and confirmed that the minor positive bias is repeatable, indicating
that the standard is reporting positive and is inherent to the standard
samples being analysed. The magnitude of the bias has been reviewed
and is deemed insignificant with respect the values being reported
(~0.02% V2O5 positive bias).
QAQC results including CRMs, duplicate samples, repeat analysis and
blanks for both Viking sample submissions and internal lab checks
show no material issues for the recent assaying programmes.
MEC Mining completed an independent audit of the Viking Mines
Database and as such have verified the significant intersections
previously reported by the Company.
No twinned holes have been drilled.
Data is collected in the field into digital devices and lo