CANEGRASS METALLURGICAL TESTWORK UPDATE
Released
Released
Announcement PDF
ASX ANNOUNCEMENT
11 September 2024
CANEGRASS METALLURGICAL TESTWORK UPDATE
•
Significant advancements made with the Canegrass Metallurgical Testwork,
focusing on improved V2O5 extraction, sulphide concentration and Titanium
separation.
•
Roasting and leaching has been completed on 5kg of magnetic concentrate from
the Stage 2 Testwork, with 15 litres of vanadium solution produced.
•
The vanadium solution is now progressing through the next steps of the flowsheet
to produce a high purity V2O5 flake and electrolyte.1
•
Stage 3 Testwork: compositing completed on an 82kg sample from the Fold Nose
Deposit, with two separate LIMS tests competed to produce magnetic concentrate.
•
•
Test 1: 40kg concentrate produced at a 150 micron grind size (delivering similar
results to the Stage 2 Testwork)2 attaining a high mass pull of 56.4%, 1.27% V2O5
for 91.6% recovery.
•
Nickel, Copper and Cobalt reported to the tail (non-magnetic fraction), with
sulphide flotation process completed to produce a sulphide concentrate.
•
0.33g/t gold identified in the sulphide rougher concentrate 1, providing
additional value opportunity for the Project to be investigated.
Test 2: 4kg of concentrate has been produced at a coarse 500 micron grind size
achieving a high mass pull of 53.9%,1.22% V2O5 grade with 81.7% recovery. This
test result is significant due to the much coarser grind size employed.
•
3.6kg of concentrate has undergone Electrostatic Separation to determine
potential for Titanium bearing Ilmenite separation.
•
Electrostatic Separation resulted in several products, but with no significant
improvement in Titanium grade.
Viking Mines Limited (ASX: VKA) (“Viking” or “the Company”) is pleased to provide an
update on the ongoing metallurgical testwork progress at the Company’s Canegrass Battery
Minerals Project (“the Project” or “Canegrass”), located in the Murchison Region of Western
Australia.
After successfully producing a Vanadium Pentoxide flake (V2O5),1 roasting of the remaining 5kg
of magnetic concentrate from the Stage 2 Testwork is now complete. 15 litres of vanadium
solution have been produced and is now undergoing the next steps in the testwork
programme designed to deliver a high-purity electrolyte and V2O5 flake.
Stage 3 metallurgical testwork is well advanced with composting and magnetic separation of
an 82kg sample now complete. Two separate tests have been completed, designed to
produce a sulphide concentrate and titanium concentrate. Gold has been identified in the
Sulphide concentrate, providing a new area of investigation for the Company.
1
2
Viking Mines (ASX:VKA) ASX Announcement 20 May 2024 - VIKING PRODUCES VANADIUM PENTOXIDE FLAKE FROM CANEGRASS
Viking Mines (ASX:VKA) ASX Announcement 6 March 2024 – VKA ACHIEVES 1.43% V2O5 & 59% FE IN HIGH QUALITY CONCENTRATE
ASX:VKA
vikingmines.com
15-17 Old Aberdeen Place
West Perth, WA, 6005
P +61 8 6245 0870
F +61 8 9322 5230
contact@vikingmines.com
1
Commenting on the progress of the metallurgical testwork, Viking Mines Managing
Director & CEO Julian Woodcock said:
“Building on the success of producing a V2O5 flake, the Stage 2 metallurgical testwork continues
to refine this process targeting the production of both a high-purity electrolyte and high-quality
flake >99% purity V2O5, which will attract a premium pricing.
“In parallel, Stage 3 testwork is well advanced, aimed at extracting additional value from the
Canegrass Project to produce concentrates of Cu, Ni, Co and Ti, using various processing
methods on both the magnetic concentrate and non-magnetic tail.
“Of significance is the identification of gold reporting to the sulphide concentrate, providing a
further valuable commodity within the Project warranting further investigation.
“These findings present additional opportunities, and I look forward to updating the market with
further results from this programme as we continue to de-risk the Project and enhance value
through this crucial testwork.”
Stage 2 Metallurgical Testwork
The Company has successfully produced a V2O5 flake from samples taken at the Fold Nose
Deposit.1 This was a critical milestone for the Company confirming the industry standard
process flowsheet can successfully be applied to the Canegrass Project material (Figure 2).
The current focus for the remaining 5kg sample from the Stage 2 Testwork is to refine and
optimise the process flowsheet and produce a high purity (>99%) V2O5 flake and vanadium
electrolyte. This is being achieved through improvements in the extraction flowsheet and
modification to the reagents used in the extraction of the Vanadium from the magnetic
concentrate.
The roasting of the remaining sample has successfully been completed, with an 89.3%
recovery of Vanadium into 15 litres of V2O5 solution. This is now undergoing further steps to
produce the high purity V2O5 flake and electrolyte. The Company anticipates being able to
provide results of the testwork in the coming months.
Figure 1; Photos showing a) Magnetite Concentrate prior to roasting, b) calcine product post roasting, and c) Vanadium bearing
solution after leaching.
ASX:VKA | vikingmines.com
2
Figure 2: Schematic flowsheet showing industry standard flowsheet stages used to process Canegrass
mineralisation with the stages completed to date (dark blue) and the stages yet to be completed (grey).
Stage 3 Metallurgical Testwork
Samples from the Fold Nose Deposit were delivered to ALS Metallurgy in Perth, Western
Australia for the Stage 3 Metallurgical Testwork programme. The focus of this programme is to
determine the possibility of producing a sulphide concentrate to recover the Cu, Ni and Co
minerals present at the Canegrass Project from the non-magnetic tail produced as part of the
Low Intensity Magnetic Separation (LIMS) process.
Additionally, the Stage 3 Testwork aims to separate the Titanium bearing mineral Ilmenite
using a method of Electrostatic Separation from the magnetic concentrate.
82kg of composite sample has now undergone two separate steps of magnetic separation,
using LIMS to produce the required material for the subsequent test stages.
Test 1: Sulphide Flotation
75kg of composite sample was prepared to a P80 150mircon (0.15mm) grind size and
processed using LIMS to produce 42kg of magnetic concentrate. The magnetic concentrate
delivered 56.4% mass pull at 1.27% V2O5 for 91.6% recovery and 11.7% TiO2 for 81.2%
recovery. Assays are still pending for the Iron grade. These results are comparable to previous
testwork2 for rougher LIMS, and it is expected that the Vanadium grade would be increased
with further regrinding and cleaning steps, however this is not the focus of this testwork.
The 33kg of non-magnetic tail has been analysed at 0.11% Cu, 0.1% Ni and 0.03% Co,
recovering 68.3%, 46.3% and 55.3% respectively.
A bulk sulphide rougher flotation step has been completed on the non-magnetic tail (Figure
3) and delivered a sulphide concentrate, demonstrating proof of concept that the Cu, Ni and
Co sulphides are amenable to be separated from the feed material.
A three-stage flotation step was employed, progressively recovering more of the Cu, Ni and
Co through each step. The composition of the rougher sulphide concentrate at each of the
respective stages are shown in Table 1 below.
ASX:VKA | vikingmines.com
3
One significant outcome from the testwork is the presence of gold reporting to the sulphide
concentrate, with 39.8% being recovered at the rougher con 1 step at a grade of 0.33g/t. A
total recovery of 50.8% of the gold was achieved through the combination of the 3 stages.
Gold has not been analysed for in the previous drilling campaigns completed at the Canegrass
Project. The presence of gold in the metallurgical testwork indicates the potential benefit of
analysing for gold in future exploration programmes at Canegrass as well as re-analysing the
pulps retained from the 2023 drilling programme to determine potential gold content in the
deposit. The Company will consider this in future work programmes.
Table 1; Table of results of the sulphide concentration testwork completed on non-magnetic tail produced as
part of the magnetic separation process for samples collected from the Canegrass Project as part of the Stage
3 metallurgical testwork.
Copper
Cobalt
%
%
recovery
%
%
recovery
%
%
recovery
g/t
%
recovery
Individual
Gold
Rougher Con 1
0.76
21.1
0.38
7.9
0.30
26.2
0.33
39.8
Rougher Con 2
0.59
12.0
0.34
5.2
0.19
12.2
0.11
9.7
Rougher Con 3
0.55
6.8
0.27
2.5
0.12
4.7
0.03
1.3
Cumulative
PRODUCT
Nickel
Rougher Con 1
0.76
21.1
0.38
7.9
0.30
26.2
0.33
39.8
Rougher Con 1+2
0.69
33.1
0.36
13.0
0.25
38.4
0.24
49.5
Rougher Con 1,2+3 0.66
39.9
0.34
15.5
0.23
43.0
0.19
50.8
Calculated Head Grade
0.08
n/a
0.11
n/a
0.03
n/a
0.02
n/a
Assayed Head Grade
0.11
n/a
0.10
n/a
0.03
n/a
0.02
n/a
Rougher Tail Grade
0.05
60.1
0.10
84.5
0.02
57.0
0.01
49.2
Figure 3; Photo showing sulphide flotation testwork being undertaken on the non-magnetic tail.
ASX:VKA | vikingmines.com
4
Test 2: Titanium Separation
7kg of composite sample was prepared using a coarse P80 500micron (0.5mm) grind size and
processed using LIMS to produce ~4kg of magnetic concentrate. A much coarser grind size
than tested previously was used as coarser material is required in the next step in the process
utilising Electrostatic Separation.
The LIMS separation has been determined to be very effective given the coarse grind size,
delivering a high 53.9% mass pull at 1.22% V2O5 for 81.7% recovery and 11.2% TiO2 for
74.9% recovery. Assays are still pending for the Iron grade. Whilst this is a lower Vanadium
recovery than the optimum levels of >90% achieved in previous LIMS testwork, it demonstrates
the potential for significant reduction in grind requirements, yet still maintaining overall high
vanadium recoveries. This will be further investigated by the company in due course.
3.6kg of the magnetic concentrate produced was subsequently processed using the
Electrostatic Separation method as a sighter test. The testwork separated the concentrate
based on the physical (magnetic) properties of the minerals, with the details of the respective
separation quantities achieved shown below in Table 2. 60% of the material reported to the
conductor, and distinctly variable quantities reporting to the M1, M2 and M3 intermediate
material types. Analysis of the differing products from the electrostatic separation is shown in
Table 3 below.
Table 2; Mass balance attained through Electrostatic Separation of magnetic concentrate.
WEIGHT
PRODUCT
Gram
%
Conductor
2,170.9
60.0
M1
1,143.2
31.6
M2
243.7
6.74
M3
48.6
1.34
Non-Conductors
10.9
0.30
3,617.1
100.0
Total
Table 3; Analysis results for different product types achieved via electrostatic separation.
Fe
PRODUCT
TiO2
V2O5
%
%
recovery
%
%
recovery
%
% recovery
Conductor
53.40
60.5
11.50
60.7
0.72
60.7
M1
52.90
31.6
11.30
31.4
0.71
31.5
M2
50.80
6.5
10.90
6.5
0.68
6.4
M3
46.50
1.2
9.87
1.2
0.61
1.1
Non-Conductors
50.00
0.3
9.85
0.3
0.66
0.3
-38µm (fines)
55.40
5.4
11.20
5.1
0.73
5.3
50.38
100.0
10.81
100.0
0.68
100.0
n/a
n/a
11.20
n/a
0.68
n/a
Calculated Head
Grade
Assayed Head Grade
ASX:VKA | vikingmines.com
5
The assay results for the different material types reveals little difference in their chemical
composition. It is interpreted that at the grind size used is not sufficient to liberate the different
mineral species in the feed material and as such has not proved effective in
concentrating/separating the Titanium contained within the concentrate.
Given the results received, the Company will not proceed with a bulk electrostatic separation
test and will revisit the results and obtain mineralogy reports to assess if other separation
methods could be effective in concentrating/separating the titanium bearing minerals found
within the Canegrass mineralisation.
NEXT STEPS
The Company is progressing through a series of metallurgical testwork programmes to further
enhance and optimise the potential process flow sheet for the Canegrass Project. These
testwork programmes will allow the Company to better understand the ore characteristics from
Canegrass and look to achieve the maximum potential value from the Project. The following
activities are ongoing:
•
Complete the processing of the Vanadium bearing solution to produce a high-purity
(targeting >99%) V2O5 flake and vanadium electrolyte.
•
Review results from Stage 3 LIMS magnetic separation which produced >46kg of magnetic
concentrate and consider the implications of grind size on future testwork programmes.
•
Investigate the source and potential of the gold identified in the sulphide concentrate to
determine potential additional product stream for the Project.
•
Investigate alternate processing methods to liberate the Titanium from the Canegrass
mineralisation.
END
This announcement has been authorised for release by the Board of the Company.
Julian Woodcock
Managing Director and CEO
Viking Mines Limited
For further information, please contact:
Viking Mines Limited
Michaela Stanton-Cook - Company Secretary
+61 8 6245 0870
Forward-Looking Statements
This document may include forward-looking statements. Forward-looking statements include, but are not limited to, statements concerning
Viking Mines Limited’s planned exploration programme and other statements that are not historical facts. When used in this document, the
words such as "could," "plan," "estimate," "expect," "intend," "may”, "potential," "should," and similar expressions are forward-looking
statements. Although Viking Mines Limited believes that its expectations reflected in these forward-looking statements are reasonable, such
statements involve risks and uncertainties and no assurance can be given that actual results will be consistent with these forward-looking
statements.
Competent Persons Statement – Metallurgical Results
The information contained in this report, relating to metallurgical results, is based on, and fairly and accurately represent the information and
supporting documentation prepared by Mr Damian Connelly. Mr Connelly is a full-time employee of METS Engineering who are a Contractor
to Viking Mines Ltd, and a Fellow of The Australasian Institute of Mining and Metallurgy. Mr Connelly has sufficient experience which is relevant
to the style of mineralisation and type of deposit under consideration, and to the activity being undertaken to qualify as a Competent Person
as defined in the 2012 Edition of the Australasian Code for Reporting of Exploration Results, Exploration Targets, Mineral Resources and Ore
Reserves. Mr Connelly consents to the inclusion in the report of the matters based on the results in the form and context in which they appear.
ASX:VKA | vikingmines.com
6
CANEGRASS BATTERY MINERALS PROJECT
The Canegrass Battery Minerals Project is located in the Murchison region, 620km north-east
of Perth, Western Australia. It is accessed via sealed roads from the nearby township of Mt
Magnet to within 22km of the existing Resources. The Project contains a large JORC (2012)
Global Inferred Mineral Resource Estimate (MRE) of 146Mt at 0.70% V2O5, 31.8% Fe & 6.6%
TiO2 (>0.5% V2O5 cut-off), see ASX announcement 20 November 2023. Viking completed a
Pit Optimisation Study (POS) on the Canegrass Global MRE, which proved highly successfully
delivering a large high-grade pit constrained MRE totalling 61Mt @ 0.81% V2O5 & 35.9% Fe,
see ASX Announcement 18 March 2024. The Fold Nose Deposit delivered the largest pit
constrained resource totalling 39Mt @ 0.81% V2O5 & 36% Fe, which the Company has opted
to make a priority target for follow up work.
PIT OPTIMISATION STUDY RESULTS – BASE CASE SCENARIO
The optimisation generates pits on each of the three deposits at Fold Nose, Kinks and Kinks
South with a breakdown provided in the Table below.
Base Case Canegrass Project MRE broken out by deposit and reported within pit constrained mineral resources.
Results are reported to JORC (2012) guidelines and are in-situ tonnage and grades
Deposit
Cutoff % JORC (2012)
V2O5 Classification
Fold Nose
Kinks
Kinks South
Total
0.7
0.7
0.7
0.7
Tonnage V2O5
(Mt)
%
Inferred
Inferred
Inferred
Inferred
39.0
15.9
6.3
61.2
Fe
%
0.81 36.0
0.77 35.5
0.85 36.7
0.81 35.9
Cu
%
Ni
%
Co
%
0.068 0.070 0.018
0.080 0.080 0.018
0.074 0.074 0.018
0.071 0.069 0.018
TiO2
%
7.6
7.4
7.8
7.6
VIKING MINES FARM-IN AGREEMENT
Viking, via its wholly owned subsidiary, Viking Critical Minerals Pty Ltd, commenced with a
Farm-In Arrangement (FIA) with Red Hawk Mining Ltd (formerly Flinders Mines Ltd) (ASX:RHK)
on 28 November 2022.
Under the terms of the FIA, Viking can acquire up to a 99% equity interest in the Canegrass
Battery Minerals Project via four farm-in stages. As of September 2024, Viking completed the
first two stages of the FIA, securing 49% of the Project.
In September 2024, the Company entered into a Share Sale Agreement (SSA) with RHK to
acquire Flinders Canegrass Pty Ltd, which holds the remaining 51% stake in the Project. With
the completion of this transaction, Viking now has 100% control of the Project.
The Project is subject to a 2% Net Smelter Royalty to Maximus Resources (ASX:MXR) which
was established when Red Hawk Mining purchased Canegrass in 2009.
ASX:VKA | vikingmines.com
7
VANADIUM REDOX FLOW BATTERIES – GREEN ENERGY FUTURE
Viking Mines recognise the significant importance of Vanadium in decarbonisation through the
growth of the Vanadium Redox Flow Battery (“VRFB’s”) sector.
VRFB’s are a developing market as an alternate solution to lithium-ion (“Li-ion”) in specific large
energy storage applications. Guidehouse Insights Market Intelligence White Paperi published
in 2Q 2022 forecasts the VRFB sector to grow >900% by 2031 through the installation of large,
fixed storage facilities (Figure 44).
Figure 4; Forecast growth of the VRFB Sector through to 2031 (source – Guidehouse Insightsi)
The reason for this forecast growth is that VRFB’s have unique qualities and advantages over
Li-ion in the large energy storage sector to complement renewable energy sources to store the
energy produced. They are durable, maintain a long lifespan with near unlimited
charge/discharge cycles, have low operating costs, safe operation (no fire risk) and have a low
environmental impact in both manufacturing and recycling. The Vanadium electrolyte used in
these batteries is fully recyclable at the end of the battery’s life.
Importantly, and unlike Li-ion, the battery storage capacity is only limited by the size of the
electrolyte storage tanks. This means that with a VRFB installation, increasing energy storage
capacity is only a matter of adding in additional electrolyte (via the installation of additional
electrolyte storage tanks) without needing to expand the core system components. Increasing
the energy storage directly reduces the levelized cost per kWh over the installation’s lifetime.
This is not an option with Li-ion batteries.
It is for these reasons that VRFB’s are an ideal fit for many storage applications requiring longer
duration discharge and more than 20 years of operation with minimal maintenance.
i) Guidehouse Insights White Paper Vanadium redox Flow Batteries Identifying Market Opportunities and Enablers Published 2Q 2022
https://vanitec.org/images/uploads/Guidehouse_Insights-Vanadium_Redox_Flow_Batteries.pdf
ASX:VKA | vikingmines.com
8
APPENDIX 2 – JORC CODE, 2012 EDITION – TABLE 1
JORC Table 1, Section 1 – Sampling Techniques and Data
JORC Code explanation
Criteria
Sampling
techniques
Drilling
techniques
Nature and quality of sampling (e.g. cut channels, random chips, or specific specialised industry standard
measurement tools appropriate to the minerals under investigation, such as downhole gamma sondes, or
handheld XRF instruments, etc.). These examples should not be taken as limiting the broad meaning of
sampling.
Include reference to measures taken to ensure sample representivity and the appropriate calibration of any
measurement tools or systems used.
Aspects of the determination of mineralisation that are Material to the Public Report. In cases where ‘industry
standard’ work has been done this would be relatively simple (e.g. ‘reverse circulation drilling was used to obtain
1 m samples from which 3 kg was pulverised to produce a 30 g charge for fire assay’). In other cases more
explanation may be required, such as where there is coarse gold that has inherent sampling problems. Unusual
commodities or mineralisation types (e.g. submarine nodules) may warrant disclosure of detailed information
Drill type (e.g. core, reverse circulation, open-hole hammer, rotary air blast, auger, Bangka, sonic, etc.) and
details (e.g. core diameter, triple or standard tube, depth of diamond tails, face-sampling bit or other type,
whether core is oriented and if so, by what method, etc.).
Method of recording and assessing core and chip sample recoveries and results assessed.
Drill sample
recovery
Measures taken to maximise sample recovery and ensure representative nature of the samples.
Whether a relationship exists between sample recovery and grade and whether sample bias may have occurred
due to preferential loss/gain of fine/coarse material.
Whether core and chip samples have been geologically and geotechnically logged to a level of detail to support
appropriate Mineral Resource estimation, mining studies and metallurgical studies.
Logging
Whether logging is qualitative or quantitative in nature. Core (or costean, channel, etc.) photography.
ASX:VKA | vikingmines.com
Commentary
RC drilling collected samples during the drilling process using industry
standard techniques including face sampling drill bit and cone splitter.
Chip samples are collected from the drill cuttings and sieved and put
into chip trays for geological logging.
Cone splitter subsamples the interval drilled and ensures that the
sample collected is representative of the interval drilled.
Reverse circulation drilling was used to obtain 1m samples which were
collected from the cone splitter. Samples have been composited in
some cases to either 2 or 4m composites by scooping from the calico
bag collected from the cone splitter at the rig. Samples were
dispatched to ALS laboratories in Perth for analysis by a XRF fused bead
analysis.
Reverse circulation drilling using a 5 ½ inch bit and a face sampling
hammer.
Recovery of sample is recorded by the field assistant when sampling and
noted as either Good, Fair or Poor. Of the samples collected from the
drilling programme, very few samples reported fair or poor recovery and
no issues were identified with sample recovery for any samples related
to the mineralised horizons.
Drilling recovery is assessed by observing sample size. Samples are
collected from the cyclone using a cone splitter and monitored for size
to determine that they are representative.
No relationship has been identified between sample recovery and
grade. This is reflected by all samples collected having a good recovery.
Further, due to the nature of the mineralisation under investigation
and the relatively high values obtained, the impact of fines is not
considered to be of significance.
All chip samples have been geologically logged to a sufficient level to
support any future mineral resource estimation, mining studies and
metallurgical studies. All chip samples are retained at the Company
offices and are available for further inspection when undertaking this
future work.
Logging of samples is qualitative in nature. Chip photos are taken of the
chip trays. All the drill spoils at the drill site are photographed to retain
a record of the colour variation within the hole.
9
JORC Code explanation
Criteria
The total length and percentage of the relevant intersections logged.
If core, whether cut or sawn and whether quarter, half or all core taken.
If non-core, whether riffled, tube sampled, rotary split, etc. and whether sampled wet or dry.
For all sample types, the nature, quality and appropriateness of the sample preparation technique.
Subsampling
techniques and
sample
preparation
Quality control procedures adopted for all subsampling stages to maximise representivity of samples.
Measures taken to ensure that the sampling is representative of the in-situ material collected, including for
instance results for field duplicate/second-half sampling.
ASX:VKA | vikingmines.com
Commentary
All metres drilled have been geologically logged.
Not applicable.
Samples were collected from the cyclone using a cone splitter for each
metre drilled in to 2 calico bags. When composite samples were
collected, a scoop is used to collect equal amounts from each metre
interval used to make the composite sample. Dry samples are
collected.
For drill samples, The sample preparation of the RC samples follows
industry best practice, involving oven drying, pulverising, to produce a
homogenous sub sample for analysis. All samples were pulverised to a
nominal 85% passing 75-micron sizing and sub sampled for assaying
and LOI determination tests. The sample preparation techniques are of
industry standard and are appropriate for the sample types and
proposed assaying methods.
For metallurgical samples, calico bags from each of the 1m samples
under investigation were collected from the field and submitted to ALS
Metallurgy in Perth, Western Australia. A master composite has been
created using ~1.5kg of sample from each of the samples provided. The
master composite sample underwent a series of magnetic separation
steps to produce a clean magnetic concentrate. Both head and tail
samples at each of the stages were analysed to determine their
composition. Analysis results of the composite compare closely to that
of the mathematically composited interval from the drilling analysis
results, supporting the appropriateness of the techniques used to
produce the composite sample. The competent person has determined
that the sample preparation technique is appropriate for the sample
types.
For drill samples, standard, blank and duplicate samples are inserted in
the sampling sequence at a rate of 1 per 20 samples (standard or blank).
This is in addition to the laboratory QAQC procedures adopted. The
quality control procedures to ensure and maximise sample
representivity are deemed appropriate.
For metallurgical testwork, Laboratory standards were used in the
analysis of the composite sample and DTR testwork samples. No issues
have been reported by the laboratory.
Drilling was conducted using a 5 ½ inch hammer to collect 1m samples.
As the style of mineralisation is massive to disseminated with results
for V2O5 being measured in %, the samples collected are deemed
representative. To monitor this, duplicate samples are collected from
the cyclone at a frequency rate of approximately 1 per 40 samples
collected (~2.5%).Samples are selected from expected mineralised
10
JORC Code explanation
Criteria
Whether sample sizes are appropriate to the grain size of the material being sampled.
The nature, quality and appropriateness of the assaying and laboratory procedures used and whether the
technique is considered partial or total.
Quality of assay
data and
laboratory tests
For geophysical tools, spectrometers, handheld XRF instruments, etc., the parameters used in determining the
analysis including instrument make and model, reading times, calibrations factors applied and their derivation,
etc.
Nature of quality control procedures adopted (e.g. standards, blanks, duplicates, external laboratory checks) and
whether acceptable levels of accuracy (i.e. lack of bias) and precision have been established.
ASX:VKA | vikingmines.com
Commentary
intervals to provide meaningful data to compare the original vs the
duplicate. Duplicate samples show a good correlation against the
original sample collected indicating that sampling is representative of
the in-situ material collected.
No duplicate samples have been prepared as part of the metallurgical
testwork programme.
The Competent Person considers the current methods and processes
described as appropriate for this style of mineralisation.
Grind size establishment testwork for the metallurgical testwork
programme showed variable grind sizes but with no apparent influence
on recovery or grade.
The nature and style of the mineralisation is relatively homogenous
and as such the sample sizes collected are appropriate to the grain size
of the material being sampled.
For drill samples, Samples were sent to ALS laboratories in Perth for
preparation and analysis. Samples were riffle split to 250g then
pulverised to a nominal 85% passing 75 microns. The Vanadium
samples underwent analysis by ME-GRA5 (H20 LOI) and MEX-XRF21u
(iron ore by XRF fusion).
For metallurgical samples, samples were analysed by ALS Metallurgy in
Perth, Western Australia. XRF method and laser ablation techniques
were used by ALS Metallurgy to analyse the samples.
The analysis methods chosen are considered appropriate for the style
of mineralisation and considered total.
Field tools were used to assist in identification of the VTM horizon for
sampling. A KT-10 magnetic susceptibility meter has been used which
measures the magnetic susceptibility of the sample. Unit specifications
are:
•
Circular coil design
•
Sensitivity: 10-6 SI units
•
Measurement range:
0.001 x 10-3 to 1999.99 x 10-3 SI units
No calibration factors are applied to the data. The duration for the
measurement sequence is 7 seconds.
As part of the drilling programme, a comprehensive QAQC programme
involving the insertion of standards (certified reference materials –
CRM’s), blanks and duplicates has been implemented. Viking inserts
standards at a frequency of 1:25, blanks 1:40 and duplicates 1:40. 3 x
CRM’s have been used by the Company which were source
Share your feedback